>Our current dilemma is that our data collected at 400C and below deviates from 
>a smooth linear trend, >and this is not expected.

In oxide perovskites the oxygen vacancies may be stabilized below the 
temperature threshold at 400-500C. It can be detected by DSC measurements.


*******************************************************
Leonid A. Solovyov
Institute of Chemistry and Chemical Technology
660036, Akademgorodok 50/24, Krasnoyarsk, Russia
http://sites.google.com/site/solovyovleonid
*******************************************************


________________________________
From: "Hudish, Grant" <ghud...@coorstek.com>
To: "Rietveld_l@ill.fr" <Rietveld_l@ill.fr> 
Sent: Wednesday, April 2, 2014 3:39 AM
Subject: Hot stage data inconsistencies 




Greetings Rietvelders,

We are currently running experiments on BCZY proton conductors.  The nature of 
the runs require us to heat our samples to 1200C, then ramp down to 800C and 
collect an Xray pattern every 25C between 800 and 400C.  We then cool in 100C 
increments and collect patterns at 300, 200, 100 & RT.

We’ve been analyzing the data in TOPAS using a whole powder pattern fitting 
procedure to obtain a cubic lattice parameter at each temperature.

Our current dilemma is that our data collected at 400C and below deviates from 
a smooth linear trend, and this is not expected.  During the fitting process 
we’re letting the lattice parameter, crystallite size, strain, and sample 
height refine.  All of these values stay consistent between temperatures except 
the sample height.  For the troubled values, we see the sample displacement 
decrease as well.

Currently, we’re not sure if this is a thermal equilibrium issue with the 
sample (unlikely) or the stage (possible?), a quark of the refinement, 
something related to our ramp rate/hold time, or loosening of the stage due to 
the extended time at temperature.  We consistently have to re-tension our Pt 
strip after each 34+hr run.

Experimental details:
Anton Paar HTK 2000N hot stage
Pt heat strip
10C/min ramp rate
10min hold at temp before scan

If anyone out there has any thoughts or criticisms on the nature of our issue 
and/or refinement method they’d be greatly appreciated!

Also, does anyone have a preferred resource/reference for hot stage XRD 
methodologies?



Grant Hudish
Materials & Ceramic Engineer
CoorsTek – Research & Development
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++             
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to