Thank everyone for all the answers (on and off)
If I can resumed all the ideas :
Question about the darkness of the pellets (could it be reduction
process ?) I should asked the student about the sintering. The ZnO is
doped with Ti/Al and Mg.
Question about the peak shift : it is true than even some nice
preparation to put the sample in the plane the peak shift could be due
to height difference.
Question about other geometrical aberration : I will try to do more
measurements with smaller Soller (0.01rad), a smaller mask 10mm and I
will fixed the sample irradiated length with the Automatic Divergent
Slit system.
Question about strain : If I am making the hypothesis that the all
sample is one phase without problem of reduction then the strain
possibility seems interesting for me.
I will give you more informations after new measurements.
Cheers, François
Le 09/12/2017 21:52, hd yahoo a écrit :
Le 12/9/2017 à 7:49 PM, N. Dragoe a écrit :
Hi
ZnO can also have a darker colour if it is obtained by thermal
treatment in low pressure of oxygen.
In my opinion, if all else is correct -I mean normal Soller slits,
correct height,… etc- there might be sample strain.
Regards
N
Le 9 déc. 2017 à 16:25, Nilesh Kulkarni <nil...@tifr.res.in
<mailto:nil...@tifr.res.in>> a écrit :
yes that is surprising. pellet is black while powder is white. ZnO
pellet should also have been white.
--
With Regards,
Nilesh Kulkarni.
----------------------------------------------------------------------------------------------------------------
Tata Institute of Fundamental Research
Department of Condensed Matter Physics and Materials Science
Room AB-88
Dr Homi Bhabha Road
Navy Nagar, Colaba
Mumbai 400005
Maharashtra, INDIA.
Phone : 91-22-22782440
Fax : 91-22-22784610
Email : nil...@tifr.res.in <mailto:nil...@tifr.res.in>
Website : http://www.tifr.res.in/~nilesh
<http://www.tifr.res.in/%7Enilesh>
XRD Website : http://www.tifr.res.in/~xrd
<http://www.tifr.res.in/%7Exrd>
----------------------------------------------------------------------------------------------------------------
Please Do Not Print This Email Unless You Really Need To.
On Sat, Dec 9, 2017 at 1:31 AM, Joachim Breternitz
<joachim.bretern...@helmholtz-berlin.de
<mailto:joachim.bretern...@helmholtz-berlin.de>> wrote:
Hi,
Given the fact that the peaks are shifted between the powder and
the pellet measurement, could it maybe be due to a height error
of the pellet during the measurement?
Best,
Joachim.
Am 8. Dezember 2017 20:48:35 MEZ schrieb Jon Wright
<wri...@esrf.fr <mailto:wri...@esrf.fr>>:
Hello,
In the photo, the pellet is black and the powder is white.
Why is that?
Best
Jon
On December 8, 2017 3:35:20 PM GMT+01:00, "François
Goutenoire" <francois.gouteno...@univ-lemans.fr
<mailto:francois.gouteno...@univ-lemans.fr>> wrote:
Dear Rietveld users,
We observe an unusual asymmetric peak shape on pellet and
not when the sample has been crushed in powder.
This asymmetry is observed even at high 2theta angle. I
would like to known if someone has an explanation ?
I have put the data in the link here after
http://perso.univ-lemans.fr/~fgouten/Asymmetry
<http://perso.univ-lemans.fr/%7Efgouten/Asymmetry>
Best Whishes, François Goutenoire
--
*********************************************************************************************
Pr. Francois GOUTENOIRE
e-mail:francois.gouteno...@univ-lemans.fr
<mailto:francois.gouteno...@univ-lemans.fr>
Tel: 02.43.83.33.54
FAX: 02.43.83.35.06
Département des Oxydes et Fluorures
Institut des Molécules et des Matériaux du Mans
IMMM - UMR CNRS 6283
Université du Maine - Avenue Olivier Messiaen
F-72085 Le Mans Cedex 9
FRANCE
*********************************************************************************************
Formation Rietveld CNRS
https://cnrsformation.cnrs.fr/stage.php?stage=18098
<https://cnrsformation.cnrs.fr/stage.php?stage=18098>
Formation SAXS et Réflectivités pour couches minces et
matériaux nanostructurés.
https://cnrsformation.cnrs.fr/stage.php?stage=18104
<https://cnrsformation.cnrs.fr/stage.php?stage=18104>
-- Diese Nachricht wurde von meinem Android-Gerät mit K-9 Mail
gesendet.
------------------------------------------------------------------------
Helmholtz-Zentrum Berlin für Materialien und Energie GmbH
Mitglied der Hermann von Helmholtz-Gemeinschaft Deutscher
Forschungszentren e.V.
Aufsichtsrat: Vorsitzender Dr. Karl Eugen Huthmacher, stv.
Vorsitzende Dr. Jutta Koch-Unterseher
Geschäftsführung: Prof. Dr. Bernd Rech (kommissarisch), Thomas
Frederking
Sitz Berlin, AG Charlottenburg, 89 HRB 5583
Postadresse:
Hahn-Meitner-Platz 1
D-14109 Berlin
http://www.helmholtz-berlin.de <http://www.helmholtz-berlin.de/>
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list
<alan.he...@neutronoptics.com <mailto:alan.he...@neutronoptics.com>>
Send commands to <lists...@ill.fr <mailto:lists...@ill.fr>> eg:
HELP as the subject with no body text
The Rietveld_L list archive is on
http://www.mail-archive.com/rietveld_l@ill.fr/
<http://www.mail-archive.com/rietveld_l@ill.fr/>
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list
<alan.he...@neutronoptics.com <mailto:alan.he...@neutronoptics.com>>
Send commands to <lists...@ill.fr <mailto:lists...@ill.fr>> eg: HELP
as the subject with no body text
The Rietveld_L list archive is on
http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list
<alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no
body text
The Rietveld_L list archive is on
http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Dear All,
2Theta shift is probably due to high adjustment. As all peaks have
this asymmetry profile it could be a contribution of low particle size
Zn-O phase, the white ZnO I think its a commercial one. Try to modify
the sample orientation and beam incidence the asymmetry in this case
will remain present.
regards,
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list<alan.he...@neutronoptics.com>
Send commands to<lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
--
*********************************************************************************************
Pr. Francois GOUTENOIRE
e-mail: francois.gouteno...@univ-lemans.fr
Tel: 02.43.83.33.54
FAX: 02.43.83.35.06
Département des Oxydes et Fluorures
Institut des Molécules et des Matériaux du Mans
IMMM - UMR CNRS 6283
Université du Maine - Avenue Olivier Messiaen
F-72085 Le Mans Cedex 9
FRANCE
*********************************************************************************************
Formation Rietveld CNRS
https://cnrsformation.cnrs.fr/stage.php?stage=18098
Formation SAXS et Réflectivités pour couches minces et matériaux nanostructurés.
https://cnrsformation.cnrs.fr/stage.php?stage=18104
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++